How to Print ASA Filament – Our Experience
We use ASA where a print has to last outdoors. At AURAPOL we make it in a wide range of colors, and here we write down what works for us when printing.
What ASA is
ASA prints similarly to ABS, but it is a bit better off. It is slightly more flexible, so it doesn't warp as much while cooling and printing is easier – the difference from ABS is not big, though. Compared to PLA, it is harder to print. In return it lasts longer in sun and rain: it doesn't fade, doesn't become brittle and doesn't deform even in a car in summer. It is suitable, for example, for:
-
holders and covers for the garden,
-
car and bike parts,
-
boxes for electronics placed outdoors,
-
signs and markings.
Before you start
-
Printer: a hotend that can handle at least 265 °C, a bed at around 110 °C.
-
Enclosed space: small prints can be done without a chamber, but we definitely recommend an enclosed chamber. If your printer doesn't have active chamber heating, turn on the bed heating in advance so the heat from the bed can warm up the chamber before printing starts. And above all, make sure there is no draft around the print.
-
Dry filament: printing from dried ASA is a must for a quality print. We dry the spools after production and vacuum-pack them, but a spool that has been lying open for a longer time should always be dried before printing. You can recognize moisture by crackling from the nozzle and a rough surface.
Print settings
In PrusaSlicer choose the Prusament ASA profile – our ASA is tuned for it. In Bambu Studio or OrcaSlicer use the Generic ASA profile.
|
Parameter |
Recommendation |
|---|---|
|
Nozzle temperature |
255–265 °C |
|
Bed temperature |
105–115 °C |
|
Cooling (fan) |
0–30%, for large parts preferably none at all |
|
Filament diameter |
1.75 mm ± 0.02 mm |
The values apply to a 0.4 mm nozzle and a speed of around 60 mm/s. Today's printers can handle much more – take 60 mm/s as slow, safe printing that gives the best quality results. At a higher speed or with a 0.6 mm or larger nozzle, increase the temperature. For small parts and slow printing, stay closer to the lower limit. Slowing down the print helps print quality a lot – if you are not in a hurry, it pays off.
First layer
ASA sticks to a smooth PEI plate very firmly and when removing it, it can tear out a piece of the surface. That's why we put a thin layer of glue stick or hairspray on the plate, which serves as a release agent.
If the print can't be removed, let the plate cool down, or put it in the fridge or freezer for a while, and then try lukewarm water.
Warping and cracking
ASA shrinks as it cools. When a print cools unevenly and too quickly, the corners lift or a tall part splits between the layers. What helps:
-
an enclosed printer,
-
the fan switched off or turned down,
-
if you print without a chamber, no draft from a window or air conditioning,
-
letting the print cool down in the chamber,
-
adding so-called “Mickey Mouse ears” to the corners of the print – small round pads in the first layer that hold the corners down on the bed and are easy to break off after printing,
-
setting a gyroid infill in the slicer.
Smell and ventilation
ASA contains styrene and releases fumes during printing. Don't print it in a bedroom or a children's room; a workshop or garage is ideal. Ventilate the room after printing, not during it. A chamber with a filter is even better.
Common problems
|
Problem |
Cause |
Solution |
|---|---|---|
|
Corners lift off the bed |
The print cools unevenly and too quickly |
Enclosed chamber, fan off or turned down, Mickey Mouse ears on the corners, gyroid infill |
|
A tall part cracked between layers |
The upper layers cool faster than the lower ones, it is cold around the printer |
Enclosed chamber preheated by the bed, less cooling, slower printing |
|
Layers are weakly bonded, the part breaks |
Low nozzle temperature, strong cooling or printing too fast |
Raise the temperature towards 265 °C, reduce the fan, slow down |
|
Strings (“cobwebs”) stretch between parts |
Temperature too high or wet filament |
Dry the filament, lower the temperature towards 255 °C |
|
The nozzle crackles, the surface is rough and matte |
Wet filament |
Dry the spool before printing |
|
The print can't be removed from the bed |
ASA sticks very firmly to smooth PEI |
Let it cool down, or use the fridge or freezer and lukewarm water; next time glue stick or hairspray |
In conclusion
In our opinion, ASA is an underrated material and many people are needlessly afraid to print it. It is enough to follow a few simple rules – dried material, an enclosed chamber and slow printing – and the results are excellent. ASA prints are strong and very durable: they withstand heat and UV radiation. On top of that, ASA can be smoothed in acetone, so you can get a beautifully smooth surface. Parts made of ASA can also be glued with acetone. If you don't know what to do, write to us.